Materials
Compare Materials
Compare candidate materials with unit-aware values and condition metadata.
| Property |
EN AW-1200 rolled sheet, 0.8 mm, directional tensile reference (CC BY experimental)
EN AW-1200 (Al 99.0) rolled sheet substrate used in a pre-painted-sheet forming study | rolled sheet
|
|---|---|
| Density |
2701.657 kg/m^3
Density
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated
|
| Thermal conductivity |
Not listed
Not listed for this material record, condition, or selected unit system.
|
| Specific heat capacity |
Not listed
Not listed for this material record, condition, or selected unit system.
|
| Young's modulus |
69.848 GPa
Young's modulus
Reported Directional Average Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated
|
| Shear modulus |
Not listed
Not listed for this material record, condition, or selected unit system.
|
| Poisson's ratio |
Not listed
Not listed for this material record, condition, or selected unit system.
|
| Yield strength |
109.096 MPa
Tensile yield strength, RD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; RD direction
107.237 MPa
Tensile yield strength, DD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; DD direction
123.172 MPa
Tensile yield strength, TD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; TD direction
113.168 MPa
Tensile yield strength
Reported Directional Average Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated
|
| Tensile strength |
125.387 MPa
Ultimate tensile strength, RD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; RD direction
117.961 MPa
Ultimate tensile strength, DD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; DD direction
134.743 MPa
Ultimate tensile strength, TD
Experimental Measured Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated; TD direction
126.03 MPa
Ultimate tensile strength
Reported Directional Average Screening
EN AW-1200 rolled sheet substrate, 0.8 mm thick; tensile coupons at 0, 45 and 90 deg to rolling direction; room temperature 20 degC; MTS 810.24 accuracy class 1; temper and sample count not stated
|
| Elongation at break |
Not listed
Not listed for this material record, condition, or selected unit system.
|
| Maximum service temperature |
Not listed
Not listed for this material record, condition, or selected unit system.
|